Showing posts with label Boatbuilding. Show all posts
Showing posts with label Boatbuilding. Show all posts

Sunday, November 15, 2026

Woodworking Tip of the Day: Fairing Board 101: Go Long, Sand at 0°, 45° and 90°

Fairing Board 101 hero illustration

Here's a Sunday-night confession from the shop. You can sand a hull till it's smooth as a baby's cheek and it can still look like a bag of walnuts the minute the first coat of gloss paint goes on. Smooth and fair aren't the same thing. Smooth is the texture. Fair is the shape. And the tool that gets you fair isn't a sander. It's a long, skinny piece of plywood with sandpaper stuck to it.

Why it matters: A random orbital or a little hand block has a short pad, so it rides down into every hollow and up over every bump and sands them all the same. You end up with a nice smooth surface that's every bit as lumpy as when you started. Gougeon's WEST SYSTEM fairing manual puts it plainly: the fairing board "should bend to the overall shape of the surface, but be long enough and stiff enough to bridge the low areas and knock down the high spots." A short block and most power tools "will simply follow the contours." Epoxyworks says the same thing: a dual-action sander leaves "a smooth but unfair surface."

Materials

  • A strip of 1/4 in. to 1/2 in. plywood, 3-1/2 in. wide. Go thinner for tight curves, thicker for flatter panels
  • Two wood scraps for handles, glued or screwed to the ends
  • Aluminum oxide or zirconia sandpaper in 50 or 60 grit and 80 grit, PSA-backed or stuck on with spray or feathering-disc adhesive
  • A soft pencil (or carpenter's chalk and a batten)
  • A good dust mask or respirator. Fairing compound dust is no joke

Tools

  • Saw to rip the plywood
  • A batten long enough to span the area you're fairing
  • Good raking light: a work light held low along the hull shows the hills and valleys
Fairing board plan: dimensions, stroke pattern, guide coat, grit sequence

Steps

  1. Build the board. Rip 1/4 in. to 1/2 in. plywood to 3-1/2 in. wide. WEST's trick is to make the length a multiple of 11 in. so sandpaper cut from 11 in. sheets goes on with no waste. 22 in. is handy for small parts, and 33 in. is about right for the topsides of a dory like the Chamberlain I've got in the shop. Glue handles on the ends for control. Big yachts use boards 4 to 6 ft long, and believe me, you'll feel those in your shoulders.
  2. Find the highs and lows first. Scribble soft pencil over the whole area, in every direction. That's your guide coat. Or rub chalk on a batten and drag it over the surface. The chalk lands on the high spots.
  3. Start coarse. WEST says to begin final fairing with 50 or 60 grit and concentrate on taking the high spots down over a broad area. Let the board do the work. Light, even pressure on both handles. Don't lean on one end.
  4. Keep changing direction. Work at 0°, 45° and 90° to the length of the panel, and both 45s. Holding one angle the whole time digs a valley. Long diagonal strokes that cross each other are the ticket.
  5. Read the pencil. Where the marks are gone, you hit a high spot or the surface is already fair. Where they're hanging on, that's a hollow. Don't chase a hollow with more sanding. You'll just dish out everything around it. Fill it with fairing compound, let it cure, scribble and sand again.
  6. Switch to 80 grit when you're close. WEST says there's no need to go finer than 80 at this stage, because the finer sanding happens after the barrier coat. If you're going to clear-finish bright wood, sand only with the grain once you're close, so you don't leave cross-grain scratches.
  7. Check with the batten. Lay it in different directions all over the surface. WEST's test: it should make solid contact everywhere, with no gaps anywhere along its length. If you see daylight under it, you're not done.

MOAM's shop note: The rookie mistake is getting tired of the long board and grabbing the orbital "just to speed things up." Twenty minutes later you've sanded right through the fairing compound on the highs and polished the lows, and you're back to square one. Save the orbital for after the shape is right. And wear the respirator. That gray dust from microballoon fairing filler gets everywhere, including places you don't want it.

Sources: WEST SYSTEM, Final Fairing & Finishing manual (board size, grit sequence, 0°/45°/90° strokes, batten check); Epoxyworks, Fairing the Bottom of Adagio (pencil guide coat, longboard vs dual-action sander).

MOAM Out.

Friday, November 13, 2026

Woodworking Tip of the Day: Roll and Tip an Epoxy Barrier Coat: Three Thin Coats, Tacky to Tacky

Roll and Tip an Epoxy Barrier Coat

Not for nuthin'…. But….. the best epoxy coat on a boat is the one you never have to sand between. I've got the dory's bottom panels ready for coating, and this is the part where a lot of guys get impatient. They slop on one fat coat with a brush, get runs, sags and a surface like an orange peel. Then they spend the weekend sanding it back off. There's a better way, and the WEST SYSTEM folks spell it right out: thin coats with a foam roller, tipped off, one on top of the next while it's still tacky.

Why it matters: A barrier coat is there to keep water out of the wood and give the paint or varnish a smooth, stable base. WEST says a minimum of two coats makes an effective moisture barrier, and three if you're going to sand it, which they recommend for most wooden boats. One coat rolled on with their thin foam roller and tipped off at room temperature (70°F) comes out around 3 to 4 mils thick. Two coats gets you 6 to 7 mils, good for most exterior surfaces. For a hull bottom that sits in the water, 9 to 10 mils is the minimum. The trick is putting coat two on while coat one is still tacky. That way the coats bond chemically, and you skip the wash-and-sand in between.

Materials

  • Epoxy resin and hardener, metered with the pumps (pick the hardener for your shop temperature)
  • Thin urethane foam roller covers (WEST 800 or similar), plus one to cut up for tipping
  • Nitrile gloves, mixing pots and stir sticks
  • For the final prep: clean water, Scotch-Brite pads, paper towels and 80-grit paper

Tools

  • A roller frame and a plastic roller pan
  • A mini roller frame for the cut-down tipping brush
  • A utility knife or bandsaw for cutting the roller cover
  • A thermometer in the shop
  • Respirator and good ventilation if the shop is closed up (see yesterday's tip)
Epoxy barrier coat plan diagram

Steps

  1. Finish everything else first. All the fairing and glass work should be done before the final coating starts. Prep the surface the way you would for bonding: clean, dry and sanded.
  2. Let the wood settle at temperature. If cold wood is warming up while you coat it, the air in the wood expands and comes out through the epoxy as bubbles. WEST calls that out-gassing. In a New England shop in November, bring the panels in and give them time to stabilize before you start.
  3. Make a tipping brush. Cut a thin foam roller cover into short segments and put one on a mini frame. WEST suggests exactly that. They say foam brushes are generally too flexible for this.
  4. Mix small and pour it out. Mix only what you can spread during its open time, and pour it into the roller pan as soon as it's mixed. Spread out in a thin layer, it stays workable longer than it does in the cup.
  5. Load the roller light. Moderate load, then roll the excess off on the ramp of the pan so the cover is evenly wet.
  6. Roll a 2 ft × 2 ft patch. Roll lightly and randomly to move the epoxy onto the area. As the roller dries out, press a little harder and spread it into a thin, even film. Thinner is better. Thin coats don't run or sag. Finish with long, light strokes and overlap the last patch to blend.
  7. Tip it off after each batch. Drag the tipping brush lightly across the fresh epoxy in long, even, overlapping strokes. Use enough pressure to knock down the stipple, but not so much that you pull the coat off.
  8. Swap the tip direction every coat. WEST's pattern is first coat vertical, second horizontal, third vertical, and so on.
  9. Recoat while it's tacky. Put the next coat on when the last one is tacky, like masking tape, but firm enough to hold the weight of the new coat. WEST says that window runs anywhere from 15 minutes to several hours, depending on the hardener and the temperature. To skip sanding between coats, get them all on the same day.
  10. Prep for paint or varnish. Let the final coat cure overnight. Then wash it with clean water and a Scotch-Brite pad to get the amine blush off, dry it with paper towels, and sand it before the finish goes on.

MOAM's shop note: If you come back and it's gone hard and you can't dent it with a thumbnail, you've missed the window. Don't roll another coat on and hope. Don't wipe it with acetone either. Blush is water soluble, so wash it with water and a Scotch-Brite, dry it, and sand any glossy spots dull with 80 grit. Then coat. When you're not sure whether it's gone too far, WEST says to play it safe: let it cure all the way, then wash and sand. And one more trick for the cold months: never thin epoxy with solvent to make it roll easier. Warm the resin and hardener up instead, and pick the right hardener for the temperature.

Three thin coats, tacky to tacky, done by suppertime. Your sanding block will thank you.

MOAM Out.

Sources: WEST SYSTEM, "Barrier Coating" and "Epoxy Chemistry" (westsystem.com); WEST SYSTEM User Manual (2020 US and 2025 EU editions); "Amine Blush & Cured Epoxy," WEST SYSTEM; "The Basics of WEST SYSTEM Epoxy Resin and Hardener," Epoxyworks.

Thursday, November 12, 2026

Woodworking Tip of the Day: Winter Shop Air: Ventilating for Epoxy and Solvents in the Cold

Wicked cold out there this week, and the shop doors are shut….. The heater's humming, the dory's on the strongback, and I'm about to wipe her down with acetone before the next coat of epoxy. That's exactly when a winter shop turns on you. In July the big doors are open and the air takes care of itself. In November everything you put in the air stays in the air, right there with you and that heater.

Why it matters: A closed-up shop is a box. Solvent and epoxy vapor build up in it. WEST SYSTEM says plainly that vapors can build up in unvented spaces, and they want ample ventilation or an organic vapor respirator. Acetone, the stuff we all wipe with, has a flash point of 0°F per NIOSH. Its vapor is heavier than air and can travel along the floor to a flame across the room. Then there's the heater itself. An unvented kerosene or propane torpedo heater puts carbon monoxide into the room, and it adds moisture and CO2 too. Those feed amine blush on your fresh epoxy. So the same heater can light the vapor, gas you, and wreck your coat. Let's fix all three.

Materials

  • Disposable nitrile gloves (neoprene, butyl or natural rubber also work per WEST). Plenty of them
  • NIOSH-approved organic vapor (OV) cartridges, black label. If you'll be sanding too, use combination OV/P100 cartridges, black and magenta (3M 60921 is one)
  • A zip-top bag or sealed container for the respirator between uses
  • Foil-backed rigid foam insulation, tape, and a light bulb or heating pad for a warm box
  • Your solvents, with the lids kept on

Tools

  • A window or box fan you can set in a window blowing out
  • A half-face respirator that fits your face
  • A battery-operated CO alarm
  • A thermometer in the shop, and one in the warm box
  • For heat while the epoxy cures: an electric heater with a thermostat and a tip-over shutoff

Steps

  1. Heat the shop first, then shut the flame heater off. Bring the shop, the boat and your materials up to temperature with whatever you've got. Then, before any thinner, acetone or solvent finish comes out, turn off every heater with an open flame or a glowing element and let it cool. Jeff Jewitt makes the same point in Fine Woodworking: stoves and heaters with an open flame or glowing element are a hazard around flammable finishes. Propane construction heater makers agree. One DESA manual says to keep the area clear of gasoline, paint thinner and other flammable vapors.
  2. Set up cross-ventilation, not a stir fan. Put the fan in a window near the work, blowing out. Crack a window or door on the far side for make-up air. Then stand so the fresh air comes past you first, across the work, and out the fan. A fan in the middle of a closed shop just stirs the vapor around and into your face. Jewitt's rule for hand-applied finishes is a fan rated in cfm about equal to the room's volume (length x width x height). A 16 x 24 shop with 8 ft ceilings is 3,072 cubic feet, so look for about 3,100 cfm. He's clear that it only works if you give the replacement air a way in, and that it isn't enough for spraying.
  3. Put on your gloves and respirator, and check the seal. Every time you put the respirator on, do the negative-pressure check from OSHA's appendix. Palms over the cartridges, breathe in gently so the mask pulls in, and hold it ten seconds. If it stays pulled in with no leak, you're sealed. Then do the positive check: cover the exhalation valve and breathe out gently. You should feel a little pressure and no air leaking at the edges. Skin is the bigger exposure with epoxy, though. WEST says skin contact is the most common way people get exposed to resin and hardener, and sensitization can come after many exposures or just one. Glenn House, Gougeon's product safety director, says a typical 4 to 6 mil disposable lasts about 30 minutes with epoxy, so change them before then, and double-glove on long jobs.
  4. Wipe or brush, then purge. Do the solvent wipe or the epoxy coat. Keep lids on the cans and get solvent rags out of the shop. Let the fan run until the smell is gone. Then close up and heat again. That's Jewitt's winter routine too: apply, vent, then close up and reheat for drying.
  5. Keep the epoxy warm instead of the whole shop. Build a box from foil-backed rigid insulation with a light bulb or heating pad inside. WEST says to keep resin and hardener at 70°F to 90°F that way. Warm epoxy pumps and mixes better and wets out better. Warm the joint itself with a heat lamp or hair dryer, or tent just that area. Know your hardener's floor. WEST 205 Fast cures down to 40°F (4°C), but slowly. 206 Slow and 207 Special Clear shouldn't be used below 60°F (16°C), and 209 Extra Slow not below 70°F (21°C). As a rule, cure time doubles for every 18°F (10C) drop.
  6. Heat for the cure without combustion in the room. If you need heat while the epoxy cures, WEST says to avoid unvented open-flame heaters that burn kerosene or fuel oil. Unburned fuel can contaminate the surface, and the extra moisture and CO2 contribute to amine blush. Turn up the thermostat, or use electric heaters or electric blankets. CPSC says an electric heater should have a thermostat and a tip-over shutoff, and to avoid ordinary extension cords. If you do run a combustion heater at other times, follow its fresh-air rule. That DESA manual calls for at least a 3 square foot opening to outside air for each 100,000 Btu/hr.
  7. Change cartridges on a schedule and store them sealed. 3M says to write the date on the cartridges when you open them, change them on a schedule, and change them right away if you can smell or taste the solvent. Between uses, store the respirator and cartridges in a sealed bag or container, away from the vapor. Even sealed, vapor can migrate through a used cartridge overnight. 3M says that for chemicals boiling below 65°C, an OV cartridge shouldn't be used longer than one shift. Acetone boils at 133°F, which is 56C. So after an acetone day, those cartridges are done.
  8. Hang a CO alarm in the shop. CPSC says unvented fuel-burning heaters pose the greatest CO threat, and mild CO symptoms like drowsiness, headaches or nausea are often misdiagnosed. A battery CO alarm is cheap. CPSC says to test alarms monthly and replace the batteries every year.

MOAM's shop note: The mistake I see most is the guy who opens a window "for ventilation" and leaves the torpedo heater roaring right next to the boat while he wipes her down with acetone. That's the worst of everything: an ignition source, CO, and a blush factory, all in one corner. Here's the trick. Do your solvent work first thing, right after you've warmed the place up and shut the heater off. The shop holds its heat long enough for a wipe-down. Then purge, close up, and let the epoxy cure under electric heat or in a tent. And never clean epoxy off your hands with solvent. WEST says not to. Use a waterless skin cleanser, then soap and warm water.

MOAM Out.

Sources: WEST SYSTEM: Preventing Overexposure WEST SYSTEM: Epoxy Safety (PDF) · Epoxyworks: Cold Weather Bonding · Epoxyworks: Let's Talk About Amine Blush · Epoxyworks: Disposable Gloves · Fine Woodworking: The Finishing Environment (Jeff Jewitt) NIOSH Pocket Guide: Acetone · ICSC 0087: Acetone · NIOSH cartridge color chart (CDPR) · 3M 60921 OV/P100 cartridge 3M: Reuse of Organic Vapor Cartridges · 3M Respirator FAQs · OSHA 29 CFR 1910.134 (Appendix B-1 seal checks) · CPSC: Space Heater Safety · CPSC: CO Alarms · CPSC: Kerosene Heater Safety · DESA propane forced-air heater manual

Tuesday, November 10, 2026

Woodworking Tip of the Day: Bottom Paint on a Wooden Boat: Hard or Ablative, Two Coats and an Extra at the Waterline

Not for nuthin'…. But.. every November the boats come out of Marblehead Harbor wearing a beard, and every April the same guys are back in the yard with a scraper, wondering why last year's bottom paint quit in August. Most of the time it wasn't the brand. It was the prep, the coat count, or the wrong kind of paint for how the boat actually lives.

Why it matters: Antifouling only works if there's enough of it, in the right places, stuck to a surface that will hold it. Interlux says it straight in their paint guide: under-applied antifouling fouls early and can cost you a mid-season haul-out. And the waterline, stem, keel and rudder edges see the most turbulence, so they wear through first. Two full coats is the floor, and those spots get a third.

Materials

  • Antifouling matched to how the boat lives: hard for trailered boats, boats stored out of the water and racers who burnish; ablative for a boat that sits on a mooring all season and should wear away slowly instead of building up (Interlux)
  • The paint maker's thinner/solvent wash (Interlux Special Thinner 216 or Brush-Ease 433; Pettit 120)
  • Primer or tie coat if the old paint is unknown or incompatible, or if you're going over bare wood with a paint that calls for one (Pettit's ECO HRT, for example, wants 6627 Tie-Coat on bare wood)
  • 80-grit paper
  • Fine-line tape for the waterline

Tools

  • Short-nap solvent-resistant roller (Interlux says 3/8"; Pettit wants 3/16" or less for ECO HRT) and a cheap wide brush for the edges
  • Sanding block, bucket and sponge for wet sanding
  • Fitted particulate respirator, nitrile gloves, eye protection and a disposable suit. Old copper paint dust is nothing to breathe or track into the house
  • Drop cloth to catch the sludge, and a stir stick. Lots of stirring

Steps

  1. Decide if you need it at all. A dory that lives on a trailer and goes in for the afternoon doesn't foul like a mooring boat. Plenty of us keep a dry-sailed boat in good bottom paint or epoxy and just hose her off. If she's staying in all summer, keep going.
  2. Pick the type to match the old paint and the use. Hard over hard, ablative over ablative is the easy road. Check the maker's compatibility chart. If you don't know what's on there, seal it with their recommended primer before you go on top.
  3. Prep the surface. Old paint in good shape: wet-sand with 80 grit and wipe with the maker's thinner. Bare wood: Interlux's ACT sheet says sand with 80 grit, wipe with 216, and thin the first coat 10% so it soaks in, then two more coats unthinned. Epoxy-coated bottom: put the first coat of antifouling on inside the primer's overcoat window (Pettit Protect is 5 to 8 hours at 70°F). Miss it and you sand the epoxy with 80 grit first.
  4. Set the waterline a little high. Run the top of the bottom paint above where she actually floats. Chop, wakes and a loaded boat ride higher than a calm day at the float. Take the gap off your own boat, not off a blog.
  5. Stir, then stir again. The biocide settles to the bottom of the can. Mix it all back in and keep stirring while you work. Thin only if the paint drags, and never more than 10% by volume (Interlux).
  6. Roll two full coats. Respect the overcoat time on the can. Interlux ACT, as an example, wants 12 hours between coats at 77°F and 50F or warmer to apply. Pacifica Plus is 4 hours. Every paint is different. The can wins.
  7. Add the extra coat where she wears. A third coat on the waterline band, the stem and forefoot, and the keel and rudder edges.
  8. Don't rush the launch. Interlux warns that skipping dry times leads to detachment, blistering or cracking. ACT is 12 hours to launch at 77F; Pettit Protect needs 72 hours after the last epoxy coat at 70°F. A cold April in Marblehead stretches all of it.

MOAM's shop note: The guy who dry-sands old copper paint with a random-orbit and no mask is in every boatyard. Don't be him. Wet-sand, wear the respirator, and catch the sludge so it doesn't go down the ramp. And one more: copper paints like ACT say right on the label not to use them on aluminum. That goes for outdrives, too.

MOAM Out.

Sources: Interlux Boat Paint Guide · Interlux ACT product sheet Interlux Pacifica Plus product sheet · Interlux: Antifouling Questions Answered · Pettit Protect application guide Pettit ECO HRT instructions

Monday, November 09, 2026

Woodworking Tip of the Day: Gluing Teak and Oily Woods: Sand Fresh, Wipe Clean, Glue Fast

Teak will humble you faster than a northeast wind on a mooring….. It's the wood every boat owner on this harbor wants on the coamings, the thwarts and the grab rails, and it's the one most likely to drop a glue joint in your lap a year later. On the Chamberlain Marblehead gunning dory I've got a few teak bits going on, and I treat every one of those glue-ups like a timed event. Because it is one.

Why it matters: The same natural oil that makes teak shrug off rot and salt also works against glue. WEST SYSTEM's own surface-prep guidance puts it plainly: wipe teak and oily woods with acetone about 15 minutes before coating, because "solvent removes the oil at the surface and allows the epoxy to penetrate." Their Epoxyworks magazine says the same thing about teak in marine work: the oils that give it durability "also work against epoxy adhesion." It isn't just teak, either. WEST lists white oak, ipe, greenheart, purpleheart and black walnut among the difficult-to-glue hardwoods. A planed face that's been sitting around is glazed and oily. Glue on that and you've glued to the oil, not the wood.

Materials

  • Teak or other oily hardwood, dry (6 to 12% moisture content, per WEST)
  • Epoxy: WEST SYSTEM G/flex 650 is their recommended pick for oily woods (1:1 by volume, about 45 minutes pot life). Standard 105-series epoxy with two-step bonding also gets used.
  • 406 Colloidal Silica if the joint is gappy, or 405 Filleting Blend for a wood-toned glue line on bright work
  • Acetone (or WEST 850 solvent)
  • Plain white paper towels. Lots of them.
  • 80-grit aluminum oxide sandpaper (no stearate "no-load" coating)

Tools

  • Sanding block
  • Shop vac or a clean bench brush
  • Mixing cups and sticks, disposable glue brush
  • Clamps and cauls, packing tape or plastic over the cauls
  • Nitrile gloves and a respirator rated for organic vapors if you're wiping much acetone in a closed shop
  • A timer. Your phone is fine.

Steps

  1. Dry-fit and mark it. Get every clamp and caul set and the parts labeled before anything gets wiped. Once the clock starts, you don't want to be hunting for the third clamp.
  2. Pre-wipe. Wipe the bonding faces with acetone on white paper towels, then dry them with fresh towels before the solvent evaporates. WEST says to clean before sanding so you don't grind the contaminant into the surface.
  3. Sand fresh. Once the solvent has flashed off, sand the bonding faces with 80-grit along the grain. You want open, fresh fibers, not a burnished planer face.
  4. Get the dust off. Vacuum or brush it with a clean brush. WEST warns against compressed air (compressor oil and water) and sticky tack rags (residue).
  5. Final wipe and start the timer. One more acetone wipe on fresh towels, wiped dry while still wet. Change towels often. Let the solvent evaporate completely, then coat within 15 minutes. That's WEST's window.
  6. Mix and coat both faces. Mix G/flex 650 1:1 by volume and coat both mating surfaces. Thicken with 406 if the fit isn't tight, or 405 if you want the glue line to blend in under varnish.
  7. Clamp light. Snug it just until a small bead squeezes out. WEST is clear on this: too much pressure squeezes the epoxy out and starves the joint. Clean up or shape the squeeze-out right away.
  8. Leave it alone. G/flex wants about 24 hours at 72°F for full cure before you stress the joint. Colder shop, longer wait. Here in a November shop in Marblehead, that means overnight and then some.

MOAM's shop note: The rag is what bites most people. WEST points out that solvent will pull silicone out of a laundered shop rag (fabric softener) and can dissolve synthetic fibers, and you end up wiping a release film onto the very face you're trying to clean. Plain white paper towels, fresh ones every pass. And keep your bare hand off the sanded face, no matter how good it looks. If you're thinking yellow glue on teak instead, Titebond's own sheets say to call their tech line before gluing oily woods. That tells you something.

MOAM Out.

Sources: WEST SYSTEM: Surface Preparation · WEST SYSTEM: G/flex 650 · WEST SYSTEM: Bonding and Clamping · Epoxyworks: Preventing Surface Contamination · Epoxyworks: Durable, Beautiful Teak

Sunday, November 08, 2026

Woodworking Tip of the Day: Epoxy Thickeners: Which Filler for Which Job

This is catching the MOAM's attention today….. the row of filler tubs on the shelf. On the Chamberlain Marblehead gunning dory I've got four or five of them going at once, and they all look like the same white-ish powder in a cup. They are not the same. One makes a joint you could hang the boat from. Another makes a putty that sands like a dream and has no business in a joint. Grab the wrong tub and you find out later, usually the hard way. So here's how I keep them straight: pick the filler for the job, then thicken it to the consistency the job needs.

Why it matters: WEST SYSTEM splits its fillers into two families. Adhesive (high-density) fillers, 404, 406, 403 and 405, cure to "a strong, hard-to-sand" epoxy plastic for bonding, fillets and hardware. Fairing (low-density) fillers, 407 and 410, cure to a "light, easily sandable material" for cosmetic work. Inside each family the fillers aren't interchangeable either. WEST's own selection guide rates each one for hardware bonding, general bonding, fillets, laminating and fairing, and the ratings move around. 404 is top dog for hardware. 406 is top for fillets. 403 is top for laminating. 410 gets no stars for anything but fairing. And the amount of filler matters as much as which one: the same cup goes from syrup to catsup to mayonnaise to peanut butter as you add powder, and each of those has its own job.

The fillers, in plain English (descriptions from WEST SYSTEM and their Epoxyworks magazine)

  • 404 High-Density: a high-strength fibrous mineral. Developed for hardware bonding where high cyclic loads are expected. Cures off-white. The hardest of the bunch to sand.
  • 406 Colloidal Silica: fumed amorphous silica (Epoxyworks notes it contains no crystalline silica). Controls viscosity and keeps epoxy from running out of vertical and overhead joints. Makes a smooth mix for bonding and fillets. WEST calls it their most versatile filler. Cures off-white.
  • 403 Microfibers: mostly cotton flock. Thickens fast, grainy "like oatmeal" when mixed, and it's WEST's go-to for bonding wood: good gap filling while still wetting into the wood fibers. Cures off-white.
  • 405 Filleting Blend: the wood-toned one, for glue joints and fillets on naturally finished wood. Cures dark brown and can be used to shade the other fillers.
  • 407 Low-Density: microballoon-based fairing filler. Easy to sand or carve, reasonably strong for its weight. Cures dark red/brown.
  • 410 Microlight: the lightest and easiest-sanding. Big fairing jobs only. WEST doesn't recommend it under dark paint or on surfaces that get hot. Cures light tan.

Generic wood flour from other suppliers works much like 405: a wood-colored structural filler for fillets and joints, often blended with silica to stop sag (TotalBoat, Jamestown Distributors).

Materials

  • Epoxy resin and its matching hardener
  • Adhesive fillers: 406 Colloidal Silica and 403 Microfibers cover most of it; 404 for hardware; 405 (or wood flour) for bright work
  • A fairing filler (410 or 407), kept on its own shelf
  • Clean mixing cups and stiff mixing sticks
  • Gloves, safety glasses and a dust mask while you're handling the powders
  • A scrap of plywood stood on edge for a consistency test

Tools

  • Disposable brush or small roller for the neat wet-out coat
  • Plastic spreader or putty knife
  • Syringe for injecting catsup-thick mix into tight spots
  • A labeled shelf or bin: adhesive fillers on one side, fairing fillers on the other

Steps

  1. Name the job before you open a tub. Is it a joint that carries load, a fillet, a bolt or fitting, a laminate, or a low spot you'll sand fair? Strength jobs get an adhesive filler. Sanding jobs get a fairing filler. That one decision keeps most mistakes off the boat.
  2. Pick the filler off the matrix. The plan above is WEST's selection guide in one chart. Glue joints, plank laps and scarfs: 403 or 406 (403 is the one WEST points at for wood). Bolts and hardware under load: 404, with 406 as the alternative. Fillets you'll paint: 406, the smoothest filleting mix. Fillets on bright wood: 405. Fairing: 410 or 407, and fairing got its own tip back in October, so I won't repeat it here.
  3. Mix the resin and hardener completely first. This is WEST's two-step rule for fillers: mix resin and hardener thoroughly, then add filler. Never stir powder into resin and then add hardener. Start with a small batch and leave room for the filler. For thick mixes, WEST says don't fill the cup more than a third full of epoxy before you add powder.
  4. Add filler a little at a time. Stir in small amounts until you reach the consistency you want, and get all of it blended before you apply it. Stir gently so the powder doesn't puff up into the air. There's no recipe to measure; WEST says to judge it by eye.
  5. Hit the right consistency for the job. WEST's four:
    • Syrup (unthickened): drips off a vertical surface. For coating, wetting out before bonding and fiberglass.
    • Catsup (slightly thickened): sags down a vertical surface. For laminating flat panels and injecting with a syringe.
    • Mayonnaise (moderately thickened): clings to a vertical surface, peaks fall over. For general bonding, filleting and hardware bonding.
    • Peanut butter (maximum thickness): clings, peaks stand up. For gap filling, fillets, fairing and bonding uneven surfaces.
    Not sure? Put a dab on the scrap of plywood standing on edge and watch what it does.
  6. For strength, don't overload it. WEST: add only enough filler to bridge the gaps without the mix sagging or running out of the joint. A small amount should squeeze out when you clamp. A stiffer glue mix isn't a stronger glue mix.
  7. Wet out first, then the thickened mix. On wood, WEST's preferred method is two-step bonding: brush neat epoxy on both faces so it soaks into the pores and end grain, then put the thickened mix on one face. You can add the filler to what's left of the wet-out batch, so mix enough for both steps. WEST says the one-step shortcut (thickened mix straight onto bare wood) isn't for highly loaded joints, especially end grain or other porous surfaces.
  8. Blend when one filler isn't quite right. WEST says fillers can be blended for in-between handling. A little 406 stiffens a mix that wants to sag, and WEST uses it to improve the consistency of other mixes. 405 shades a mix darker. For bright work, Epoxyworks suggests thickening with 406 and adding a little sanding dust from the same wood to match the color.

MOAM's shop note: Color is the one people forget until the varnish goes on. 404, 406 and 403 all cure off-white. On a painted hull nobody cares. On bright work, an off-white glue line or fillet shows like a chalk line on mahogany. On the dory, anything that'll be varnished gets 405 or 406 tinted with sanding dust from the same plank, and I test the color on a scrap first. The other thing: keep the fairing tubs on a different shelf from the glue tubs. 410 in a structural joint is a mistake you won't see until the boat's working in a chop off Tinker's Island.

Sources: WEST SYSTEM, Filler Selection Guide and individual filler pages (403, 404, 405, 406, 407, 410); WEST SYSTEM User Manual & Product Guide (2020 US edition: fillers, four consistencies, two-step filler rule, one-third-full cup, two-step and single-step bonding, hardware bonding); WEST SYSTEM User Manual (March 2025 edition: filler characteristics ratings for sanding); Epoxyworks, "The Basics of WEST SYSTEM Epoxy Resin and Hardener" (what each filler is made of, two-step bonding, 406 plus sanding dust for color) and "Furniture Building Tips"; TotalBoat, "Epoxy Fillers Guide"; Jamestown Distributors, "Which filler should I use for my epoxy project?" Ratings are WEST's for WEST products; other brands' fillers differ, so check your own maker's chart.

MOAM Out.

Thursday, November 05, 2026

Woodworking Tip of the Day: Paint Over Epoxy: Wash, Sand and Prime So the Topcoat Sticks

This is catching the MOAM's attention today….. the day the epoxy finally cures hard on a hull panel and somebody reaches for the paint can. On the Chamberlain Marblehead gunning dory, that barrier coat of epoxy is only half the job. Paint protects the epoxy from sunlight, and the epoxy gives the paint a stable base. Together they last a lot longer than either one alone. But paint does not stick to glossy, blushy epoxy. You wash, you sand, you prime when the system calls for it, and then the topcoat goes on. Skip a step and you get fish-eyes, peeling, or a finish that never quite dries.

Why it matters: WEST SYSTEM's finish guidance is blunt: before paint or varnish, the epoxy surface has to be clean, dry and sanded. Amine blush, that waxy film that shows up when epoxy cures in cool, damp air, will clog sandpaper and kill adhesion if you leave it. Solvents don't take it off. Water does. And once the epoxy is fully cured, paint adhesion is mechanical — the film keys into the sanding scratches. Too fine a grit and there isn't enough tooth. Paint the wrong system over a dirty surface and you're scraping it next spring.

Materials

  • Fully cured epoxy on the work (not the soft, tacky gel stage)
  • Clean water and a Scotch-Brite pad (WEST calls out the 7447 general-purpose pad)
  • Plain white paper towels
  • Aluminum oxide sandpaper in the grit your coating wants (no stearate-coated paper)
  • Primer if the paint maker calls for it — high-build for filling scratches, or a two-part epoxy primer such as Interlux Epoxy Primekote under Brightside
  • The topcoat itself: marine enamel, one-part urethane, two-part LP, varnish, or bottom paint as the job requires
  • A scrap test panel coated the same way as the boat

Tools

  • Bucket, scrub pad, and fresh rinse water
  • Random-orbit sander or a sanding block; vacuum or brush for dust
  • Optional: wet/dry paper if you want to wash and sand in one pass
  • Roller and tip-off brush, or spray gear if the coating allows it
  • Gloves, eye protection, and whatever respirator the paint label requires

Steps

  1. Let the last epoxy coat cure fully. The green, tacky recoat window is for epoxy on epoxy. Before paint, varnish, primer or gelcoat, WEST says let the epoxy cure hard, then wash and sand. Cool shops and slow hardeners can take days. If a one-part paint won't dry over it, unfinished cure is a common reason.
  2. Wash the blush off first. Scrub with clean water and a Scotch-Brite pad. Dry with paper towels while the surface is still wet so the dissolved blush comes off on the towel instead of drying back down. WEST says plain water is enough; soap, ammonia or bleach can leave their own film. Interlux allows warm water and a little all-purpose soap — if you use soap, rinse hard. Change the wash water. Don't reach for acetone: Interlux and WEST both say aggressive solvents don't remove amine blush.
  3. Then sand. Paint grips the scratches. Start at 80 grit if you have runs, sags or leftover gloss after the wash. For a high-build or filling primer, WEST says 80–100 grit is usually enough. For most primers and high-solid coatings, 120–180 grit. For a high-gloss paint or varnish, finish at 220–400. Grits finer than that may not leave enough tooth. Always finish at the grit the coating maker lists. Wet-sanding removes blush and dust in one pass if you prefer that route.
  4. Rinse and check the water break. After you're happy with the fairing, rinse with fresh water. The water should sheet evenly. If it beads or fish-eyes, you've still got contamination — wipe with solvent and a paper towel, wet-sand again, and recheck. Vacuum or brush off dry dust; skip sticky tack rags on epoxy (WEST warns the residue can cause fish-eyes).
  5. Coat soon. WEST's tip: start the primer or paint within about 24 hours of the final sanding so the surface doesn't pick up shop film again. The surface has to be thoroughly dry.
  6. Prime when the system wants it. WEST says primers are usually not required for adhesion on epoxy — the paint keys into the sanding scratches — but high-build primers are useful for hiding scratches and fairing marks, and some bottom paints want their own interface primer. Self-etching primers don't work on cured epoxy. For Interlux Brightside over clear epoxy, the Brightside data calls for washing off amine blush, sanding with 80 grit, then one to two coats of Epoxy Primekote before the topcoat. Interlux also prefers a two-part primer over a single-part Pre-Kote when blush is a concern, because blush can migrate through one-part primers and spoil the cure of Brightside.
  7. Apply the topcoat per the can. Follow the maker's recoat windows, sanding between coats, and temperature range. WEST ranks two-part linear polyurethanes as the most durable UV protection over epoxy; alkyds and one-part urethanes are easier but less tough, and some one-part urethanes fight amine-cure epoxy (WEST notes 207 Special Clear Hardener can help compatibility — test). Bottom paints are usually fine over a prepared epoxy barrier; use only primers rated for below the waterline under them.
  8. Make a test panel. WEST and the paint makers both say it: a scrap piece coated and prepped the same way as the boat tells you whether your wash, grit and primer actually stick before you commit the hull.

MOAM's shop note: Wash first, sand second. Every time. Sanding a blushy surface just grinds the wax into the scratches, and then no amount of primer saves you. On a cool, damp Marblehead week, assume blush is there even when the panel looks glossy and clean. One wash at the end of the epoxy schedule beats three peeling seasons.

Sources: WEST SYSTEM, "Final Epoxy Surface" (final surface prep, grit ranges, 24-hour coating window, water-break rinse); WEST SYSTEM, "Surface Preparation" (amine blush wash with water and Scotch-Brite 7447, wash-before-sand, full cure before non-epoxy coatings); WEST SYSTEM, "Finish Coatings" (UV role of paint over epoxy, primer guidance, self-etching primers, coating types, test panel); Epoxyworks, Joe Parker, "Comparing Surface Prep Techniques for Paints and Primers" (Awlgrip 545 / Brightside adhesion test; 80-grit under primer, 120-grit on primer); Interlux, "What is amine blush…" (wash before sanding; solvents don't remove blush; Brightside / Pre-Kote / Epoxy Primekote notes); Interlux Brightside data (clear epoxy: remove blush, 80 grit, Epoxy Primekote, then Brightside). Check your own product data sheets for recoat times and final grit.

MOAM Out.

Wednesday, November 04, 2026

Woodworking Tip of the Day: Gluing End Grain: Why It Starves and How to Size It First

Gluing end grain: size it first

Not for nuthin'…. But….. the joint that looks the best coming out of the clamps is sometimes the weakest one in the whole piece, and it's almost always the one where the end of a board meets something else. End grain. You brush on glue, clamp it up, wipe it clean, and it looks great. Then the corner lets go, and the face of the joint looks dry. I'm building a Chamberlain Marblehead gunning dory and I've been a licensed contractor long enough to have seen miters, butt joints and plank ends open up. So today: why end grain starves a joint, how to size it with yellow glue, how to prime it with epoxy, and the real fix, which is to stop relying on it at all.

Why it matters: Franklin, the company behind Titebond, explains it with a drinking straw. Gluing end grain is like gluing the ends of two straws together instead of the sides. There's much less wood surface for the glue to grab, and most of what you're looking at is air. Worse, a thin glue can be drawn down the open pores by capillary action, which leaves a starved joint, or the end grain can suck the water out of the glue so fast it dries before you get the parts together. Fine Woodworking's Matthew Kenney says the same about a miter: end grain "sucks up glue like crazy" and will starve the joint long before the glue has a chance to dry.

And even a well-prepped end-grain joint has a ceiling. The USDA Forest Products Laboratory's Wood Handbook says it is practically impossible to make an end-grain butt joint strong enough for ordinary service with conventional bonding techniques, and that even with special techniques a butt joint only reaches about 25% of the tensile strength of the wood along the grain. A well-made scarf, finger or lap joint can reach up to 90%. That's the whole point of today's tip: sizing helps, and for light-duty work it's plenty, but the strong joint is the one where the glue meets long grain.

Materials

  • Yellow glue (PVA) suited to the job, plus water and a small cup for the size
  • Epoxy resin and hardener, with a filler (colloidal silica or microfibers) for the thickened coat
  • A thicker glue, if you want that route (Titebond No Run, No Drip is made for end grain and miters)
  • Painter's tape or packing tape for light clamping on miters
  • Clean, freshly cut end grain. Sand or plane it right before you glue it, and keep oil and finish off it

Tools

  • A sharp saw, plane or shooting board, so the joint closes with no gaps
  • Cheap brushes (acid brushes are fine) for the size and the glue
  • Mixing sticks and a clean mixing cup for epoxy
  • A damp rag or a putty knife for squeeze-out
  • Optional: a heat gun for gently warming the wood before the epoxy wet-out
  • Clamps, or tape, to hold the joint with light, even pressure
Plan: sizing and gluing end grain

Steps

  1. Ask first: do I have to glue end grain? Titebond's own tip begins by admitting that good joint design minimizes the need for gluing end grain, though sometimes it's unavoidable. For ends that have to join end to end, use a scarf, finger or lap. The Forest Products Lab says solid wood wants a slope of 1 in 12 or flatter for the highest strength, and 1 in 8 is typical for plywood. For an end meeting the edge of another piece, the Lab says a plain end-to-edge joint has a hard time carrying much load, and recommends interlocking joints so edge grain bonds to edge grain: dowels, mortise and tenons or rabbets.
  2. Make it fit. A size can't fill a gap. Kenney's point is that if the joints are tight, you get a good glue line and a strong joint. Dry-fit it, and fix the cut, not the glue.
  3. Mix the size. Titebond's mix is one part glue to one to two parts water. Fine Woodworking and Franklin's technical presentation both say 50/50 glue and water, which is inside that range. Brush it on the end grain only.
  4. Decide how long to let it work. Titebond's tip says let it soak in no more than two minutes, then continue with a regular application of glue. Kenney and Franklin's presentation describe a size that soaks in and dries first, plugging the pores, and then you glue normally. Both end up in the same place, which is pores that are plugged before the full-strength glue goes on. If you go the dry route, plan the wait into the glue-up so you aren't sizing and gluing in a rush.
  5. Glue it normally. Put full-strength glue on, fit the parts, and watch your open time (it depends on the glue and the temperature). Franklin's presentation says the point of the size is that the end grain then doesn't drink the glue or dry it out before assembly. If you don't want to size, the other route is a thicker glue: Franklin lists Titebond No Run, No Drip at about 36,000 cps against about 4,000 cps for most wood glues, and says it sets with minimal clamping.
  6. Clamp it lightly and wipe squeeze-out. End-grain joints on small boxes and frames often get tape instead of clamps. Kenney points to a painter's tape trick for miters. One reader on his post notes that tape can hide squeeze-out, which is hard to clean off a crisp miter later, so wipe it before you tape.
  7. With epoxy, wet out first. For end grain, WEST SYSTEM says use two-step bonding. Brush unthickened epoxy onto both mating faces, and re-wet very porous surfaces and end grain, because they soak it up. WEST says single-step bonding (thickened epoxy straight on both faces) shouldn't be used for end grain or other porous surfaces, and that neat epoxy keys into end grain better than thick epoxy.
  8. Then the thickened coat. Stir filler into your mix until it's thick enough to bridge gaps, put it on one surface before the wet-out epoxy cures (WEST's 2020 manual says before it's no longer tacky), and clamp with just enough pressure to squeeze a small amount out, about a firm hand grip. Too much pressure can squeeze it all out and starve the joint.
  9. Give the epoxy a warm start. WEST's Wooden Boat manual notes that warming the wood with a heat gun makes epoxy thinner so it penetrates more deeply into exposed end grain. Gougeon Brothers' crew did the same on mast scarfs, pre-warming the joints before priming them with unthickened epoxy because wood that is cooling draws epoxy into the grain. Keep the heat gentle and the wood well short of scorched.
  10. Add glue area where you can. WEST's manual says the three things behind joint strength are the glue, the adhesion and the joint area, and that increased overlap, scarf joints, fillets and reinforcing fibers all add bonding area. An epoxy fillet in an inside corner also acts as a structural brace.

MOAM's shop note: Sizing is a fix for starving, not for geometry. If the joint carries a load, or has to live through a wet winter on a boat, change the joint, not the glue. Scarf it, lap it, tenon it, or fillet it. And don't clamp harder to make up for a dry joint. Squeezing won't put back glue the end grain already drank.

Sources: Titebond (Franklin International), "Did you know? Get good results gluing end grain joints" (titebond.com, Woodworking Glues, application tips); Franklin / Titebond presentation, "A Word on End Grain Gluing"; Matthew Kenney, "Not all miters need reinforcement," Fine Woodworking, Feb. 27, 2015; USDA Forest Products Laboratory, Wood Handbook, Chapter 10 (FPL-GTR-190), "End-Grain Joints" and "End-to-Edge-Grain Joints"; WEST SYSTEM, "Bonding and Clamping," the Epoxy Problem Solver, the WEST SYSTEM User Manual (2020), and the Restoration & Repair (Wooden Boat) manual; Epoxyworks, "Choosing Glue!" (Russell Brown). Open times, clamp pressure and ratings vary by product, so check the data sheet for your glue.

MOAM Out.

Tuesday, November 03, 2026

Woodworking Tip of the Day: Measuring Epoxy Right: Mix Ratios, Pumps and Why 'Close Enough' Fails

Measuring Epoxy Right: Mix Ratios, Pumps and Why Close Enough Fails

Pull up a stool….. this is the least glamorous step in epoxy work, and it decides whether the rest of the job lives or dies. Nobody brags about measuring. But most of the sticky, gummy, "why won't this cure" stories start right here, and WEST SYSTEM says so too: most problems with the curing of epoxy can be traced to the wrong ratio of resin and hardener. Winter is coming, the shop is cold, and I'd rather scrape nothing off the dory this year.

Why it matters: Epoxy isn't paint that dries. It's two parts that react with each other, and the reaction only finishes if the right amounts meet. An Epoxyworks article from WEST SYSTEM's technical staff puts it this way: with excess hardener, hardener molecules stay unreacted in the cured epoxy and weaken it, and they can keep later paint coats from setting up. Too little hardener is no better. WEST says too much or too little hardener affects both the cure time and how thoroughly it cures. That's why their manual says, in capital letters, not to adjust the cure time by changing the ratio. If you want it faster or slower, pick a different hardener. The ratio stays put.

Materials

  • Resin and the hardener made for it (same system, same brand)
  • Matching calibrated pumps, or a scale, or straight-sided graduated cups
  • Clean mixing containers: plastic, metal or wax-free paper (not glass, not foam)
  • Mixing sticks with a flat end
  • A stiff plastic or metal scraper and a solvent for the bad-batch day
  • Gloves, safety glasses and paper towels
  • Your product's data sheet, because the numbers below are WEST SYSTEM's and other brands differ

Tools

  • 300 Mini Pumps (or a gram scale, or a stick marked in equal parts)
  • Roller pan, for coating jobs, to get the mix out of the cup
  • A small test cup for the pump check
Plan: epoxy mix ratios, pumps, mixing and bad-batch cleanup

Steps

  1. Read the ratio off your hardener. With WEST SYSTEM 105 Resin, the 205 Fast and 206 Slow hardeners are 5 parts resin to 1 part hardener by volume. The 207 Special Clear and 209 Extra Slow are 3 to 1. The pumps are matched to the hardener, so a 205/206 pump and a 207/209 pump aren't interchangeable, and the group size (A, B or C) has to match too. Other makers use other ratios: System Three Clear Coat is 2 to 1 by volume, and MAS LV resin is 2 to 1. Check your product's data sheet.
  2. Prove the pumps once. If equal full strokes are going in, the resin and hardener containers should run empty at about the same time. WEST's pump sheet also says to mix a small test batch and watch it: it should cure to a hard solid, overnight at room temperature or warmer. Epoxyworks suggests 3 strokes each, stirred thoroughly, left until fully cured. Do it with new pumps, and again any time curing acts up.
  3. One full stroke of resin for each full stroke of hardener. Push the head all the way down, then let it come all the way back up before the next stroke. WEST says partial strokes give the wrong ratio. Same number of strokes from each pump, every batch. In a cold shop the pumps move thicker material, so press slowly and give them extra time to return. Keep the resin and hardener at room temperature if you can.
  4. No pumps? Measure carefully. By volume, use a container with straight sides and a square inside corner, graduated or marked with a stick, and pour the resin first. Epoxyworks points out it's easier to see the space for the hardener that way. By weight, don't use the volume numbers. The weight ratios are different because the resin and hardener have different densities. For WEST 105, the data sheets give 5.19 to 1 (205), 5.36 to 1 (206), 3.64 to 1 (207) and 3.68 to 1 (209). Per 100 g of resin, that's roughly 19.3 g, 18.7 g, 27.5 g and 27.2 g of hardener. The manual rounds 205/206 to "five parts resin to one part hardener" and 207/209 to 3.5 to 1 by weight, which sit inside the data sheets' acceptable ranges. Use the data sheet, though. That's why the plan has a table.
  5. Stir at least a minute and scrape as you go. WEST's US instructions say at least 1 minute, longer in cooler temperatures. Their March 2025 manual's figure says 2 minutes. In a November shop I go with the longer one. Scrape the sides and bottom, and use the flat end of the stick to get into the inside corner. Unmixed resin hiding in the corner is how you get a soft spot. MAS Epoxies makes the same point about soft spots, and adds a pouring tip: don't scrape the last drips and film off the walls of the cup onto your work, since that's the part that might not be mixed.
  6. Thicken after, never before. WEST's manual calls it a two-step process: mix the resin and hardener thoroughly first, then blend in the filler in small amounts. Their problem solver says the same thing: only add fillers or additives after the resin and hardener have been thoroughly mixed.
  7. If it's still tacky when it should be hard, think before you recoat. If the shop is cold, epoxy cures slower, so allow extra time and add gentle heat (WEST warns that unvented kerosene or propane heaters can inhibit the cure and contaminate the surface). If it was off ratio or under-mixed, waiting won't fix it.
  8. Remove the bad batch. WEST says don't apply more epoxy over non-curing epoxy. Warm it to lower its viscosity and scrape off as much as you can with a stiff metal or plastic scraper. Clean the residue with a solvent (WEST's current manual names its 850 Cleaning Solvent), with plenty of ventilation. Let the solvent dry before you recoat, then recoat with a fresh batch.
  9. Find out why before you mix again. Equal full strokes? The right pump for the hardener (5:1 or 3:1) and the right group size? Pump ratio checked? Resin and hardener from the same system? WEST's list also includes wrong products: resin won't cure properly with other brands of hardener.

MOAM's shop note: "Close enough" has a real meaning, and it isn't eyeballing. WEST's data sheets publish an acceptable ratio range by weight for each hardener (4.83 to 6.20 to 1 for 105/205, for example), and it's wider on the resin-rich side. Calibrated pumps used with full, equal strokes keep you comfortably in it. A cup poured by eye, a half-pumped stroke, or a "splash more hardener to speed it up" is how you end up outside it. If you slip, err toward a little extra resin, not extra hardener. Epoxyworks says the same about a pump that spits air. Then write the hardener, ratio and pump strokes on the shop wall once, and stop doing the math on the fly.

Sources: WEST SYSTEM, "Dispensing and Mixing" and "Epoxy Problem Solver" (westsystem.com); WEST SYSTEM User Manual & Product Guide (2020 US edition and March 2025 edition); WEST SYSTEM 300 Mini Pump Instructions; WEST SYSTEM data sheets for 105/205, 105/206, 105/207 and 105/209; Epoxyworks, "Getting the Most out of Mini Pumps" (Jim Derck, GBI, 1995); System Three, Clear Coat product page and data sheet; MAS Epoxies, "The Ultimate Guide for Mixing Epoxy Resin" and 2:1 LV resin page; Entropy Resins technical video, "Mix Ratio: Measuring and Mixing Epoxy". Ratios and mixing times differ by product, so check your own data sheet.

MOAM Out.

Monday, November 02, 2026

Woodworking Tip of the Day: Bandsaw Safety: Guide Height, Hand Zone, Relief Cuts and Round Stock

Bandsaw Safety woodworking tip of the day

This is catching the MOAM's attention today….. the bandsaw is the friendly one in the shop. It cuts down toward the table, so it doesn't throw stock back at your belt buckle like a table saw can. That's exactly why people get casual with it. But the blade is still an open strip of steel running at full speed, and almost every bandsaw story starts with a hand that wandered into the wrong spot. Here's the short list I run through, pulled from the saw makers' own manuals and the woodworking magazines.

Why it matters: Popular Woodworking points out that a bandsaw's cutting force is aimed at the table, which all but eliminates kickback toward you. It can still drag small offcuts down into the throat plate, and a bad cut can snap the blade or pull it off the wheels. The Grizzly manual says dull blades take more effort and raise the risk of accidents, and OSHA's woodworking rules call for pulling dull, badly set or improperly tensioned saws out of service before they start to jam or kick back.

Materials

  • A sharp blade that suits the job, not cracked and with no missing teeth
  • Safety glasses, hearing protection and a dust mask or respirator
  • A push stick or two, and a shop brush for the table
  • A V-block or cradle jig for any round stock
  • Your saw's owner's manual (yes, really, because the numbers differ)

Tools

  • The bandsaw, unplugged for setup
  • A pencil for the layout line
  • A shop vac or dust collector hooked up
Bandsaw safety plan: guide height, hand zone, relief cuts, V-block

Steps

  1. Unplug it and check the blade. Teeth point down toward the table. Look it over for cracks and missing teeth before every use. Grizzly says not to run a dull, cracked or badly worn blade. Fine Woodworking's tell for a dull one is that it takes extra pressure to cut, runs hotter and leaves a dark end on the kerf. Make sure the wheel covers are closed.
  2. Set tension and guides. Tension to the scale for the blade width, as your manual says. Grizzly's 14" saw fine-tunes it by backing the tension off until the blade just flutters, then going 1/4 turn tighter. Set the guides and thrust bearing close to the blade without touching it. Grizzly says about 0.016" behind the blade (four thicknesses of a folded dollar bill) and Laguna says about 1/16" behind the teeth.
  3. Drop the upper guide to about 1/4" above the stock and lock the post. Laguna, Grizzly's 9" saw, and the University of Washington shop all say 1/4". Popular Woodworking says 1/4" or less, since a guide set too high leaves the blade unsupported and it can twist. Rikon says 1/8" to 1/4". Be aware that Grizzly's 14" manual allows up to 1", and Fine Woodworking's curve-cutting article uses 1/2" as a gap that still blocks your fingers from passing under. Follow your manual, and keep it as low as the cut allows.
  4. Plan the cut so you never back out of a curve. Match the blade width to the radius. Fine Woodworking says a 1/2" blade won't make a 1" radius. For a tight curve, make relief cuts first from the waste edge, stopping just short of the line and about an inch apart. The waste falls away in small pieces and the blade doesn't pinch. Backing out of a short straight cut is OK, but not out of a curve, where the stock can catch the back of the blade and pull it off the wheels.
  5. Suit up. Glasses, hearing protection, and a dust mask, with the dust collector running. Laguna, Rikon and Grizzly all list these.
  6. Set your hand zone. Popular Woodworking says to keep your hands outside a 3" boundary around the blade and the guide/guard. The University of Washington shop says at least 2" to the side of the blade and never in front of it. I go with 3". Hold the stock flat on the table with your hands off to the sides. Never put your fingers in line with the blade. Narrow or small pieces get a push stick, jig or vise. Scraps on the table get a brush or a stick, never your fingers.
  7. Round stock goes in a V-block. A dowel on the bare table is unsupported where the blade bites it, so it spins and drags your fingers in. The University of Washington says to hold round or cylindrical pieces in a V fixture, and Popular Woodworking says to V-block all round stock. Betty Scarpino wrote in American Woodturner that a dowel as small as 1/4" can break a blade. Keep your hands at the outer ends of the jig, well off the cut line.
  8. Start and cut. Switch on and let it come to full speed first. Never start with the work touching the blade. Feed evenly with light pressure, and don't twist the blade around small curves. If the motor is dragging, you're feeding too fast. Lightly cupped boards go cupped side down on the table. Grizzly says not to cut badly warped stock at all.
  9. Stop it, then fix it. To back a piece out of a curve, jammed scrap or a broken blade: switch off and let the blade stop on its own. Don't try to slow it with your hand or the wood. Unplug it before you reach into the table slot to clear a jam. When you're done, wait for a full stop, unplug, brush off the table and, if it's going to sit, release the blade tension (Grizzly and Laguna both say this saves blade and saw).

One more thing on stance: Popular Woodworking says the blade, if it breaks and flies off the wheels, tends to whip to the right as you face the saw. Facing the blade is the usual stance. Keep a balanced footing, and don't stand in the whip path when you don't have to.

MOAM's shop note: The easy mistake is raising the guide for one tall cut and then leaving it up for the next skinny one. It takes five seconds to drop it, and that's the difference between a blade that's guarded and supported and one that's waving around in the open. Do it every cut, along with the glasses and the push stick. The number of times I've heard "I only needed one quick cut" is the reason these rules exist.

Sources: Laguna V10 Bandsaw owner's manual; Grizzly Model W1706 14" and W1878 9" bandsaw manuals; Rikon 10-324TG 14" bandsaw manual; University of Washington Woodshop band saw safety procedures; Popular Woodworking, "Band Saws" (2008); Fine Woodworking, "How to Cut Flawless Curves on the Bandsaw"; Betty Scarpino, American Woodturner (Feb 2016); OSHA 29 CFR 1910.213 (bandsaws and inspection and maintenance of woodworking machinery). OSHA's rules are written for workplaces; they're still good sense in a home shop.

MOAM Out.

Bandsaw Safety woodworking tip of the day

This is catching the MOAM's attention today….. the bandsaw is the friendly one in the shop. It cuts down toward the table, so it doesn't throw stock back at your belt buckle like a table saw can. That's exactly why people get casual with it. But the blade is still an open strip of steel running at full speed, and almost every bandsaw story starts with a hand that wandered into the wrong spot. Here's the short list I run through, pulled from the saw makers' own manuals and the woodworking magazines.

Why it matters: Popular Woodworking points out that a bandsaw's cutting force is aimed at the table, which all but eliminates kickback toward you. It can still drag small offcuts down into the throat plate, and a bad cut can snap the blade or pull it off the wheels. The Grizzly manual says dull blades take more effort and raise the risk of accidents, and OSHA's woodworking rules call for pulling dull, badly set or improperly tensioned saws out of service before they start to jam or kick back.

Materials

  • A sharp blade that suits the job, not cracked and with no missing teeth
  • Safety glasses, hearing protection and a dust mask or respirator
  • A push stick or two, and a shop brush for the table
  • A V-block or cradle jig for any round stock
  • Your saw's owner's manual (yes, really, because the numbers differ)

Tools

  • The bandsaw, unplugged for setup
  • A pencil for the layout line
  • A shop vac or dust collector hooked up
Bandsaw safety plan: guide height, hand zone, relief cuts, V-block

Steps

  1. Unplug it and check the blade. Teeth point down toward the table. Look it over for cracks and missing teeth before every use. Grizzly says not to run a dull, cracked or badly worn blade. Fine Woodworking's tell for a dull one is that it takes extra pressure to cut, runs hotter and leaves a dark end on the kerf. Make sure the wheel covers are closed.
  2. Set tension and guides. Tension to the scale for the blade width, as your manual says. Grizzly's 14" saw fine-tunes it by backing the tension off until the blade just flutters, then going 1/4 turn tighter. Set the guides and thrust bearing close to the blade without touching it. Grizzly says about 0.016" behind the blade (four thicknesses of a folded dollar bill) and Laguna says about 1/16" behind the teeth.
  3. Drop the upper guide to about 1/4" above the stock and lock the post. Laguna, Grizzly's 9" saw, and the University of Washington shop all say 1/4". Popular Woodworking says 1/4" or less, since a guide set too high leaves the blade unsupported and it can twist. Rikon says 1/8" to 1/4". Be aware that Grizzly's 14" manual allows up to 1", and Fine Woodworking's curve-cutting article uses 1/2" as a gap that still blocks your fingers from passing under. Follow your manual, and keep it as low as the cut allows.
  4. Plan the cut so you never back out of a curve. Match the blade width to the radius. Fine Woodworking says a 1/2" blade won't make a 1" radius. For a tight curve, make relief cuts first from the waste edge, stopping just short of the line and about an inch apart. The waste falls away in small pieces and the blade doesn't pinch. Backing out of a short straight cut is OK, but not out of a curve, where the stock can catch the back of the blade and pull it off the wheels.
  5. Suit up. Glasses, hearing protection, and a dust mask, with the dust collector running. Laguna, Rikon and Grizzly all list these.
  6. Set your hand zone. Popular Woodworking says to keep your hands outside a 3" boundary around the blade and the guide/guard. The University of Washington shop says at least 2" to the side of the blade and never in front of it. I go with 3". Hold the stock flat on the table with your hands off to the sides. Never put your fingers in line with the blade. Narrow or small pieces get a push stick, jig or vise. Scraps on the table get a brush or a stick, never your fingers.
  7. Round stock goes in a V-block. A dowel on the bare table is unsupported where the blade bites it, so it spins and drags your fingers in. The University of Washington says to hold round or cylindrical pieces in a V fixture, and Popular Woodworking says to V-block all round stock. Betty Scarpino wrote in American Woodturner that a dowel as small as 1/4" can break a blade. Keep your hands at the outer ends of the jig, well off the cut line.
  8. Start and cut. Switch on and let it come to full speed first. Never start with the work touching the blade. Feed evenly with light pressure, and don't twist the blade around small curves. If the motor is dragging, you're feeding too fast. Lightly cupped boards go cupped side down on the table. Grizzly says not to cut badly warped stock at all.
  9. Stop it, then fix it. To back a piece out of a curve, jammed scrap or a broken blade: switch off and let the blade stop on its own. Don't try to slow it with your hand or the wood. Unplug it before you reach into the table slot to clear a jam. When you're done, wait for a full stop, unplug, brush off the table and, if it's going to sit, release the blade tension (Grizzly and Laguna both say this saves blade and saw).

One more thing on stance: Popular Woodworking says the blade, if it breaks and flies off the wheels, tends to whip to the right as you face the saw. Facing the blade is the usual stance. Keep a balanced footing, and don't stand in the whip path when you don't have to.

MOAM's shop note: The easy mistake is raising the guide for one tall cut and then leaving it up for the next skinny one. It takes five seconds to drop it, and that's the difference between a blade that's guarded and supported and one that's waving around in the open. Do it every cut, along with the glasses and the push stick. The number of times I've heard "I only needed one quick cut" is the reason these rules exist.

Sources: Laguna V10 Bandsaw owner's manual; Grizzly Model W1706 14" and W1878 9" bandsaw manuals; Rikon 10-324TG 14" bandsaw manual; University of Washington Woodshop band saw safety procedures; Popular Woodworking, "Band Saws" (2008); Fine Woodworking, "How to Cut Flawless Curves on the Bandsaw"; Betty Scarpino, American Woodturner (Feb 2016); OSHA 29 CFR 1910.213 (bandsaws and inspection and maintenance of woodworking machinery). OSHA's rules are written for workplaces; they're still good sense in a home shop.

MOAM Out.

Sunday, November 01, 2026

Woodworking Tip of the Day: Flattening Your Sharpening Stones: Pencil Grid, Lapping Plate and How Often

Woodworking Tip of the Day: Flattening Your Sharpening Stones

Not for nuthin'…. But….. the sharpest-looking set of stones in a lot of shops is also the reason the chisels won't pare a clean shaving. Waterstones wear every time you use them, and they wear the most right in the middle. Nobody notices until the plane iron comes off the stone with a rounded edge and a back that won't lap flat. I've got a dory's worth of bevels, gains and frames to cut this winter, so I went back to the stone makers' own instructions and the Fine Woodworking and Popular Woodworking articles and wrote down how I keep mine flat.

Why it matters: A waterstone cuts fast because its binder lets go and keeps exposing fresh abrasive. The price is that it dishes. Shapton says it plainly: the blade hits the middle of the stone more often, so the stone goes concave, and that makes for uneven sharpening. Tom Caspar wrote in Popular Woodworking that the wear "produces an undesirable curved edge on chisels and plane irons." It's worse on the back of a blade. Lay a flat back on a hollow stone and it only touches the high ends, so lapping it there rounds it over instead of flattening it. Paul Sellers' answer to that problem is to lap backs on something that stays flat, like a diamond plate or thick glass. A sharp edge is where two faces meet, and a dished stone spoils both of them.

Oilstones vs. waterstones: Norton says its oilstones (benchstones) "typically do not require flattening with normal use" because they're hard, but after years of steady use they can dish in the spots where you bear down the most. Waterstones are the other way around: they dish easily, but they're quick to bring back. Same job, different schedule.

Materials

  • Your sharpening stones, every grit (not just the coarse one)
  • A soft pencil
  • Water, plus a tub or a sink without a garbage disposal (DMT says the slurry is hard on disposal bearings)
  • Rags and a stiff nylon brush for cleanup

Tools: pick one flattener

  • Diamond lapping plate. The DMT Dia-Flat (DMT is out of Marlborough, Mass.) is 10" × 4", ground flat to ±0.0005", and comes in 120 micron for stones of 1000 grit and coarser or 95 micron for finer stones. An Atoma plate is 140x or 400x diamond on a 10 mm aluminum block, flat to ±0.04 mm (about 0.0016"). Lee Valley suggests the 400x for general truing and the 140x when you need to take off a lot fast.
  • Coarse diamond stone. Lee Valley says a coarse (about 400x) metal-backed diamond plate makes a good flattener and doubles for grinding a primary bevel. There's a catch, though. DMT doesn't recommend its regular sharpening plates for lapping stones, only the ones marked Dia-Flat, and Deneb Puchalski (Fine Woodworking) warns that some diamond stones wear out of flat fast. If you use one, keep it just for lapping.
  • Silicon carbide grit on glass. Lee Valley's lapping kit says to true stones with 90x or 180x and finish with 280x, on plate glass, with water as the only lubricant for waterstones. Their guide calls for glass at least 1/4" thick, supported on flat plywood or MDF so it can't flex. A plastic laminate sheet on the glass keeps the grit from dishing the glass itself. (Don't use loose grit on a steel plate for waterstones. Lee Valley says the oxides from a wet ferrous lap will ruin the stone.)
  • Wet/dry sandpaper on glass or granite. It's the cheapest way in. Norton says 100 grit, Charlesworth used 180 or 240 on 1/2" float glass, and Caspar used 220 on plate glass 1/4" or thicker. Lee Valley also lists coarse aluminum oxide sheet (over 100 micron) on glass or granite. Sellers' advice for a flat granite tile is to take a straightedge to the store and pick through them until you find a flat one.
  • Grooved silicon carbide flattening stone. Norton recommends one. Soak it and the waterstone, then rub them together, and the grooves carry the slurry away.
  • Shapton's Diamond Glass Lapping Plate is only for stones of 500 grit (30 micron) and finer. Don't use it on coarse stones, don't put loose grit on it and don't run hot water over it.
  • A good straightedge
Plan: flattening sharpening stones

Steps

  1. Wet everything. Soak your soaking stones the way the maker says. Shapton says to give its stones 2 to 3 minutes before lapping and to let other brands soak up all the water they can hold. Set the plate or glass on something solid and flat, and splash it with water.
  2. Draw a pencil grid across the whole face of the stone. Fine Woodworking, Lee Valley and Shapton all start this way. The pencil shows you what the stone is doing.
  3. Lap with long figure-8 strokes. DMT says to use long, overlapping figure-8s with light to moderate pressure and the whole plate, and to finish lighter so you leave fewer scratches. Shapton's way, forward and back and then both diagonals, works just as well. Turn the stone end for end now and then. Keep it wet, and rinse the slurry out of the plate's grooves as it builds up.
  4. Read the grid. The lines go first on the high spots. On a dished stone that's the ends and edges, and the middle hangs onto its lines the longest. When every line is gone, the stone is flat. Lee Valley says not to fuss if it doesn't quite reach the corners, since that's the part of the stone that matters least.
  5. Check it with a straightedge. Lay it along the length, the width and both diagonals and hold the stone up to the light. If any light shows under it, go back to the plate.
  6. Chamfer the edges. Caspar sands a 45° bevel on every edge of the stone "to prevent flaking." Charlesworth eased the soft edges so they wouldn't crumble. Touch them up after each flattening, since lapping leaves a sharp corner again.
  7. Do every stone. The 1000, the 4000 and the 8000 all wear, just at different rates. Rinse and brush each stone before you go to the next grit so coarse grit doesn't ride along and scratch up your finish stone. If you'd rather lap stone against stone, use three and keep rotating them. Lee Valley warns that rubbing just two together can leave one concave and the other convex.
  8. Clean up the flattener. DMT says to clean and dry the Dia-Flat after every use, and to scrub any diamond plate now and then with a nylon brush and a mild cleanser. Lee Valley says to wipe the swarf out of an Atoma's channels. Put a straightedge across your plate or glass once in a while too, because a flattener that isn't flat just copies its own error into every stone.

How often? More often than you'd think. Lee Valley says to lap waterstones every 3 to 5 minutes of use. Shapton says to lap every time you sharpen a blade. Charlesworth flattened his 800 after about 100 strokes of back work, and Caspar flattened his three stones before every session, which he said took a minute or so. Plenty of folks flatten at the end of each session so the stones are ready the next time. Oilstones are on a much longer clock: check them with the straightedge now and then and flatten when they show a dish. The rule is little and often. A stone that's barely off comes back in a minute, and a badly dished one costs you a lot of stone.

One for the New England shop: Charlesworth warns not to store waterstones in water if the shop freezes at night, "because the stones will shatter." Come December in an unheated Marblehead shop, my soakers come in the house or get stored dry.

MOAM's shop note: The mistake I see most is flattening the 1000 and calling it done. The finish stone dishes too, just slower, and it's the last stone that touches your edge. The second most common is the fella who flattens only when he can see the hollow. By the time you can see it, you've already rounded a few irons. Draw the grid, lap it out, knock off the edges, and keep your flattener clean and flat. A few minutes, and every stone on the bench is flat.

Sources: DMT Dia-Flat product page and DMT FAQ, Lee Valley's Atoma Diamond Plates page, Lapping Grits instructions, "Getting Started with Japanese Water Stones," "Care and Maintenance of Ceramic and Water Stones" and Sharpening by Hand guide, Shapton Diamond Glass Lapping Plate instructions and FAQ, Norton "A Guide to Waterstones" and "A Guide to Benchstones," David Charlesworth, "A User's Guide to Waterstones" (Fine Woodworking #169), Deneb Puchalski, "Flatten Waterstones with a Coarse Diamond Stone" (Fine Woodworking #224), Hendrik Varju, "Pencil and Paper" (Fine Woodworking), Tom Caspar, "Waterstones" (Popular Woodworking / American Woodworker), and Paul Sellers, "Sharpening on hollow stones."

MOAM Out.